Wet filament causes more "my printer is broken" posts than anything else: stringing, popping, bubbles, rough surfaces and weak layers. Here are the starting points I use in a hobby filament dryer. Always check the manufacturer's label first, because some brands publish their own numbers.
- PLA: 45–50 °C, 4–6 hours. Don't go much hotter: PLA softens around 55–60 °C and the spool or the filament can deform.
- PETG: 60–65 °C, 4–6 hours.
- TPU / flexibles: 50–55 °C, 4–6 hours. TPU absorbs moisture fast, so dry it right before printing.
- ABS / ASA: 65–80 °C, about 4 hours.
- Nylon (PA) and nylon-CF: as hot as your dryer goes, up to about 80 °C, for 8–12 hours. Nylon gets wet within hours in humid rooms, so print straight from the dryer if you can.
- PC and PC blends: 70–80 °C or your dryer's maximum, 6–8 hours.
Things worth knowing
- Many cheap dryers top out somewhere between 55 and 70 °C, and the air around the spool is usually cooler than the number on the display. If the material needs more heat than your dryer gives, run it longer.
- Drying doesn't help filament that has gone brittle with age. If it snaps when you bend it after drying, it's done.
- Storage matters as much as drying. Sealed bins or vacuum bags with silica gel desiccant keep dried spools dry for weeks.
- A cheap hygrometer in your storage box tells you when the desiccant needs recharging.
What dryer are you using, and have you found settings that work better for a specific brand?