PETG strings more than PLA, and most of the fixes people pass around are in the wrong order. This is the order that has worked for me. Change one thing at a time and print a small stringing test between steps.
1. Dry the filament first. This is the cause most of the time. If you hear popping or crackling from the nozzle, or see tiny bubbles and a rough surface, it's wet. About 65 °C for 4–6 hours in a filament dryer usually does it. Then store it in a sealed box with desiccant. No setting will fix wet PETG.
2. Lower the nozzle temperature. Drop it 5 °C at a time (most PETG prints somewhere between 230 and 250 °C; check the label). A temperature tower makes this quick. Stop when layer adhesion starts to get weak.
3. Calibrate pressure advance / linear advance. Most modern printers and slicers have a calibration test for this. If it's way off, the nozzle keeps oozing after every move.
4. Then tune retraction. Direct-drive extruders usually want short retractions (roughly 0.5–1.5 mm), and Bowden setups longer ones. Going further than you need can make things worse by pulling molten plastic up into the cold zone.
5. Cut down travel over open space. Turn on "avoid crossing walls/perimeters" (the name varies by slicer) and wipe on retract if you have it. Fewer jumps across open air means fewer strings.
6. Keep the nozzle clean. PETG collects on the outside of the nozzle and drags across the print. Brush it while it's hot with a brass brush before starting.
A few fine wisps are normal with PETG. A quick pass with a heat gun or hair dryer on high takes them off in seconds.
What fixed it for you? Post your printer and filament and what made the difference.